Gnee Steel (tianjin) Co., Ltd
+8615824687445

What Is a High-Quality Cold Rolled Steel Sheet? EN 10130 Grades, EN 10131 Tolerances and Inspection Guide

Aug 25, 2023

 

Products Description

 

Cold rolled steel is one of the most widely specified flat products in the world - as the base for stamping and deep drawing, and as the substrate for galvanized, galvalume and prepainted (PPGI/PPGL) products. "High quality" is not a marketing word: it is a combination of measurable properties defined by standards such as EN 10130, EN 10131, JIS G3141 and ASTM A1008. This guide explains how a professional buyer judges CR sheet quality, with the actual numbers.
Cold rolled steel
Cold rolled steel

How Cold Rolled Steel Sheet Is Made

 

Hot rolled strip is pickled to remove scale, then cold reduced in a tandem mill (typically 40-90% reduction), annealed (batch or continuous) to restore ductility, and finally skin-passed (temper rolled) to control yield-point behavior and surface roughness. The sheet is then oiled and cut to coil or sheet. Each step shows up in the final product: pickling quality in surface, mill setup in flatness and gauge, annealing in mechanical properties, and skin pass in surface finish and forming behavior.
 

The Six Dimensions of Quality

 

1. Surface Quality
EN 10130 defines two surface appearance classes. Appearance A allows slight pores, scratches, marks and staining that do not affect formability or coating; Appearance B requires one face essentially free of defects so that paint or electrolytic coating looks uniform. Surface finish is graded by roughness Ra: shiny "b" (Ra ≤ 0.4 µm), semi-shiny "g" (Ra ≤ 0.9 µm), normal "m" (0.6 µm < Ra ≤ 1.9 µm) and rough "r" (Ra > 1.6 µm). If not specified, material is supplied with Appearance A and normal finish. A high-quality sheet is free of scratches, dents, pits, rolled-in scale, rust stains and coil-break lines.
 
2. Thickness and Dimensional Tolerances (EN 10131)
EN 10131:2006 sets normal and special tolerance classes for thickness, width, length, flatness, camber and out-of-square for cold rolled products (0.35-3 mm). Thickness tolerances depend on nominal thickness, width and the yield-strength family. Examples for the most common family (minimum yield strength below 260 MPa, width ≤ 1200 mm, normal class):

 

Nominal thickness (mm)
Normal tolerance (mm)
Special tolerance (mm)
0.40 < t ≤ 0.60
±0.03
±0.025
0.60 < t ≤ 0.80
±0.04
±0.030
0.80 < t ≤ 1.00
±0.05
±0.035
1.00 < t ≤ 1.20
±0.06
±0.040
1.20 < t ≤ 1.60
±0.08
±0.050
1.60 < t ≤ 2.00
±0.10
±0.060
2.00 < t ≤ 2.50
±0.12
±0.080
2.50 < t ≤ 3.00
±0.15
±0.100
Width tolerance (sheets/wide strip ≥ 600 mm, normal): 0/+4 mm up to 1200 mm width; length tolerance 0/+6 mm below 2 m and 0/+0.3% above. Tolerances widen for higher-strength families and for special orders - always confirm the class in the order. Verify with supplier.
 
3. Mechanical Properties and Formability (EN 10130)
 
EN 10130:2006 covers DC01-DC07, in rising order of formability. Key values (elongation A80 applies to product thickness ≥ 2 mm and decreases with thinner gauges - see the standard):
Grade
EN No.
C max (%)
Yield Re (MPa)
Tensile Rm (MPa)
A80 min (%)
Typical use
1.0330
0.12
140-280
270-410
28
General forming
1.0347
0.10
140-240
270-370
34
Drawing
DC04
1.0338
0.08
140-210
270-350
38
Deep drawing
DC05
1.0312
0.06
140-180
270-330
40
Extra deep drawing
DC06
1.0873
0.02
120-170
270-330
41
Super deep drawing (IF steel)
For drawing grades, EN 10130 also specifies minimum plastic-strain ratio r90 and strain-hardening exponent n90 (e.g. DC06 r90 ≈ 1.9-2.1, n90 ≈ 0.20 for applicable thicknesses). Values are thickness-dependent - confirm against the mill certificate. A "high-quality" sheet delivers consistent values across the whole coil, not just at the head.
 
4. Chemical Composition Consistency
Low carbon content is what makes CR sheet formable: carbon drops from 0.12% max (DC01) to 0.02% max (DC06), with tight P/S/Mn limits. A quality mill reports heat-analysis chemistry on the certificate and keeps variation low between heats - chemistry drift is a common hidden cause of cracks in deep drawing. Ask for a chemistry breakdown per heat when consistency matters.
 
5. Flatness and Edge Quality
EN 10131 limits out-of-square to 1% of sheet width, and camber (lapping) to 5 mm over a 2 m base. Flatness (edge wave / center buckle) is limited by tolerance class and is tighter for thin, wide sheet. Edges must be cleanly cut without burrs or cracks, especially for slitting. Measure a few sheets diagonally on receipt if flatness-critical parts are planned.
 
6. Inspection, Certification and Packaging
High-quality material ships with an EN 10204 Type 3.1 mill test certificate (chemistry + mechanical results), is measured for thickness at the normal position (coil) or 15 mm from the edge (sheet), and is protected with rust-preventive oil plus VCI paper and moisture-barrier wrapping. Rust stains on delivery are an immediate quality red flag.

 

Global Grade Cross-Reference

 

Common mappings (approximate - always confirm against the mill certificate):
EN 10130
JIS G3141
ASTM A1008
China GB/T 5213
Formability level
DC01
SPCC
CS Type B
DC01
Commercial / general forming
DC03
SPCD
DS Type B
DC03
Drawing
DC04
SPCE
DDS
DC04
Deep drawing
DC06
SPCG (IF)
EDDS
DC06
Super deep drawing

 

Request Latest Steel Price Today

 

Receiving Inspection Checklist

 

1.Verify the mill certificate: standard, grade, heat numbers, chemistry and mechanical results (EN 10204 3.1).
2.Measure thickness at several points across the width; compare with the ordered tolerance class.
3.Visual check: scratches, dents, pits, rust, oil stains, edge burrs, coil breaks.
4.Check surface roughness Ra with a portable profilometer if finish is critical.
5.Run a sample bending/forming test for drawing grades; watch for Lüders lines or orange peel.
6.Confirm packaging: oiling, VCI paper, moisture barrier, edge protection.
7.Any value not covered by the certificate: mark "Verify with supplier" before acceptance.
 

Frequently Asked Questions

 

1.Which cold rolled grade should I choose for deep drawing?
DC04 is the standard deep-drawing grade under EN 10130; use DC05 for extra deep drawing and DC06 (IF steel, max 0.02% C) for the most severe draws. Higher grades give better r90/n90 values but lower yield strength - match the grade to the part, not to the price.
 
2.What thickness tolerance can I expect for 0.5-1.0 mm cold rolled sheet?
Under EN 10131 normal class (Re < 260 MPa, width ≤ 1200 mm): 0.40-0.60 mm → ±0.03 mm; 0.60-0.80 mm → ±0.04 mm; 0.80-1.00 mm → ±0.05 mm. Special class is about 20-30% tighter. Confirm the class in the order - it changes the price.
 
3.Why is skin-passing (temper rolling) important?
Skin-passing after annealing removes yield-point elongation, preventing Lüders lines (stretcher strains) during forming, and controls surface roughness and flatness. It is a key difference between stamping-grade and general-purpose sheet.
 
4.Does cold rolled steel rust?
Yes. Bare CR steel has no inherent corrosion resistance; it is shipped oiled with VCI protection and will rust quickly once exposed to moisture. Long-term protection requires galvanizing, galvalume or PPGI/PPGL coating.

 

Summary

 

High quality cold rolled steel sheets are steel sheets that have excellent properties, meet stringent standards and meet the needs of a variety of applications. The following are some characteristics of high quality cold rolled steel plates:

 

Excellent surface quality: the surface is flat, smooth, no defects, cracks, dents and so on.

Precise dimensional control: Conforming to the specified size and thickness tolerances ensures stable use in a variety of processes and applications.

High strength and toughness: with enough strength and toughness, can withstand external load and strain, not easy to deformation or fracture.

Good formability: it can carry out complex forming and processing, and is not easy to crack, deformation or fracture.

Stable chemical composition: Has a consistent chemical composition to ensure the stability and predictability of the material's performance.

High corrosion resistance: with good corrosion resistance, can be used in different environmental conditions for a long time, not easy to rust or corrosion.

Low internal stress: After proper heat treatment or annealing, it can reduce or eliminate internal stress and improve the stability of the material.

Comply with relevant standards: comply with international, national or industry standards, such as ASTM, EN, JIS, etc., to ensure product quality and performance meet the specified requirements.

Reliable quality inspection: Strict quality inspection and testing in the production process, including dimensions, surface quality, chemical composition, mechanical properties and so on.

Suitable for a variety of applications: it can adapt to the needs of different fields such as construction, automobile manufacturing, home appliances, industrial equipment, etc.