Bubble
The bubbles mentioned here refer to the surface bubbles generated during the extrusion process of industrial aluminum profiles, rather than those caused by casting porosity. Of course, casting porosity may be a contributing factor, but it is by no means a decisive factor. Casting porosity may form a large number of bubbles on the surface of aluminum profiles during quenching heat treatment after extrusion. The bubbles generated by extrusion remain in their original state during quenching and will not develop again.
Generation of Squeezing Bubbles: When there is a large gap between the ingot and the extrusion cylinder, the extrusion stage begins, that is, during casting and upsetting. If the ingot cannot be deformed from front to back and the air in the gap is expelled from the extrusion cylinder, it is possible to form compressed bubbles between the cylinder wall and the surface of the ingot, and the pressure inside the bubbles increases with the increase of extrusion pressure. At the same time, friction occurs between the ingot and the extrusion cylinder wall, or between the plastic deformation zone and the dead zone of the compression cone, resulting in shear deformation and tensile stress on the surface of the ingot or the outer circumference of the compression deformation cone, which may form instant small cracks. When compressed bubbles under immense pressure meet such small cracks, the compressed bubbles may break through the shell and invade the microcracks. After extrusion, it is stretched and deformed, forming bubbles on the surface of industrial aluminum profiles. The sound of "explosion" can sometimes be heard when compressed bubbles burst. The larger the gap between the ingot and the extrusion cylinder, the more severe the wear of the extrusion cylinder and the extrusion pad, the faster the upsetting speed, or the more volatile gas generated when lubricating oil is carried into the extrusion cylinder, the greater the probability of surface bubbles forming during extrusion. This type of bubble sometimes changes from large to small in a straight line distribution along the direction of compression. Reduce the gap between the ingot, extrusion pad, and cylinder wall, and reduce the amount of air remaining in the extrusion cylinder; Prevent lubricant contamination of the extrusion cylinder; Especially, gradient heating along the length direction is applied to the ingot, and the upsetting speed at the beginning of the extrusion stage is appropriately slowed down to achieve the deformation of the ingot from front to back, and air is discharged from the extrusion cylinder, effectively avoiding or reducing the generation of extrusion bubbles.
In addition, when the split die is extruded, extrusion bubbles will be generated on the next profile at the junction of industrial aluminum profiles. This type of bubble generally occurs on the upper surface of aluminum profiles. Due to the separation of scraps and the cutting of them from top to bottom, the exposed scraps outside the mold are removed and dropped, while the excess metal connected to the profile in the split mold cannot be removed, leaving space above the mold hole. When squeezing the next profile, the upset ingot seals and pressurizes the gas in the upper space of the mold hole, leaving bubbles on the upper surface of the profile head. Of course, if the separation shear enters from the side, bubbles will be left on the side where the separation shear enters. The slow upsetting speed of these bubbles can be slightly reduced, but it is difficult to completely eliminate them. However, these types of bubbles are generally not too severe and only appear at the head. After cutting, they are not harmful to use and have an impact on the yield, but the impact is not significant.